Slake Durability Test | Procedure, Measurements, Calculations and Classification

Поделиться
HTML-код
  • Опубликовано: 13 сен 2024
  • Testing procedure, measurement, calculations and classifications are given below.
    This test is performed on rock to estimate its durability to weathering (mechanical disturbance and effect of water). For this test, about 500g of rock samples/pieces (each about 40-60g) are used. The slake durability index obtained for the second cycle is used to classify rock.
    Test measurements and calculations from the test in this video are as follows:
    Mass of empty drum (m4) 842.2 g
    Mass of drum with rock sample (m1) 1285.5 g
    Mass of drum with dried rock after 1st cycle (m2) 1244.6 g
    Mass of drum with dried rock after 2nd cycle (m3) 1237.1 g
    Calculations of slake durability index for 1st (Id1) and second (Id2) cycles:
    Id1=(m2-m4)/(m1-m4)=(1244.6-842.2)/(1285.5-842.2)=402.4/443.3=0.907 or 90.7%
    Id2=(m3-m4)/(m1-m4)=(1237.1-842.2)/(1285.5-842.2)=394.9/443.3=0.891 or 89.1%
    Based on Id2, durability of this rock is 'Medium High' (see the table below).
    Classification table based on slake durability index
    Durability Id1 Id2
    Very High 99-100 98-100
    High 98-99 95-98
    Medium High 95-98 85-95
    Medium 85-95 60-85
    Low 60-85 30-60
    Very Low less than 60 0-30
    Reference: Franklin, J. A., & Chandra, R. (1972, May). The slake-durability test. In International Journal of Rock Mechanics and Mining Sciences & Geomechanics Abstracts (Vol. 9, No. 3, pp. 325-328). Pergamon.
    Other rock mechanics laboratory tests:
    Unconfined compression test • Unconfined Compression...
    Schmidt Hammer Test | Testing Procedure on How to Measure Rock Strength in Field • Schmidt Hammer Test | ...
    Schmidt Hammer Test | Part 2: Data analysis • Schmidt Hammer Test | ...
    Point Load Test • Point Load Test | How ...
    Rock Quality Designation Index (RQD) • How To Measure Rock Qu...
    How To Measure Rock Surface Roughness with Profilometer (Barton Comb) • Easy Way To Measure Ro...
    Tilt Test to Measure Friction between Two Rock Surfaces • How to Measure Frictio...
    Slake durability test • Slake Durability Test ...

Комментарии • 11

  • @Pancake8274
    @Pancake8274 2 года назад +3

    This channel is a gem. Thank you sir for your hardwork.

  • @ercieyyy
    @ercieyyy 2 года назад +3

    I'd like to remind that the first measurement of the rock samples before the first cycle should be taken as oven-dried according to the standards

  • @stephanieivyluna4042
    @stephanieivyluna4042 2 месяца назад

    salute to you sir!

  • @eng.saberabdulla9996
    @eng.saberabdulla9996 Год назад

    Thank you for sharing this test

  • @jacobmachayuenmalok4737
    @jacobmachayuenmalok4737 Год назад +1

    thanks for your well explanation but why is it important to determine the dispersion strength indices of rock samples?

  • @ishwarsingh4193
    @ishwarsingh4193 2 года назад

    U r awesome..! Sweet person..! With excellent videos..,

  • @grahamlloyd7157
    @grahamlloyd7157 Год назад

    Excellent!

  • @joserobertosalgueiro2228
    @joserobertosalgueiro2228 Год назад

    Thanks

  • @BabyEnginee0
    @BabyEnginee0 Год назад

    Thanks sir

  • @mspathak7641
    @mspathak7641 2 года назад

    Was the rock sample used oven dried?

  • @zahraumj
    @zahraumj Год назад

    applause