Smelting PC Parts for GOLD and PALLADIUM | Mix Computer Parts Gold recovery

Поделиться
HTML-код
  • Опубликовано: 14 мар 2024
  • Gold and palladium recovery from mix PC parts
    Components:
    Motherboards, RAMs, CD-ROMs, Hard drive, Graphic cards, Dial up card, Sound card, CPUs
    Please subscribe to my RUclips channel by ➰clicking on Link below 👇
    ❌ Your support will aid me in creating higher-quality videos:❌
    👇
    ruclips.net/user/PickyPlans?su...
    Contact me on :
    Instagram : / pickyplans
    Facebook: / picky.plans
    telegram: t.me/pickyplans
    #goldrecovery
    #smelting
    #cupellation
    #ewasterecycling
    #makingmoney
    #gold
  • РазвлеченияРазвлечения

Комментарии • 69

  • @PickyPlans
    @PickyPlans  2 месяца назад +3

    8kg (16 PCs) motherboards mix mostly 1 BGA
    9 PCS DDR RAMs mostly 1 sided ICs
    5 PCS CD ram boards
    6 PCS Graphic cards with BGA
    7 PCS voice cards
    1 piece Hard PCB

    • @edibandulan5266
      @edibandulan5266 2 месяца назад

      Wait is that striping powder is Cyanide the deadly poison that also use to disolve gold? I never see people strip gold really easy like this, they often burn this and wash with nitric acid to remove silver and copper.

  • @OwlTech333
    @OwlTech333 2 месяца назад +5

    Wow in this video you managed to cover all aspects of PM extractive metallurgy!

    • @PickyPlans
      @PickyPlans  2 месяца назад +1

      You are the only one who has referred to this.

    • @noureddineroman8884
      @noureddineroman8884 Месяц назад

      There is a better and faster way 😊😅

    • @Amac-uz9hm
      @Amac-uz9hm Месяц назад +1

      @@PickyPlans i was thinking that exact same thought, i have been thinking of alllll the seperate ways of extraction and you just did it in one video, outstanding!!!! where do you get the stripping powder ??

    • @PickyPlans
      @PickyPlans  Месяц назад +1

      Thank you my friend...
      Seems only legends know these...
      BTW, I make it myself. It's my product...

    • @Amac-uz9hm
      @Amac-uz9hm Месяц назад

      @@PickyPlans what country are you friend?

  • @Amac-uz9hm
    @Amac-uz9hm Месяц назад +1

    outstanding

  • @irwanmochammad1174
    @irwanmochammad1174 2 месяца назад

    Great... Always succes ..boss..👍👍😂🙏

  • @ImanGoldRecovery
    @ImanGoldRecovery 2 месяца назад

    excellent video brooo

    • @PickyPlans
      @PickyPlans  2 месяца назад

      Thank you so much bro🙏❤️

  • @pasqualemicillofilho8049
    @pasqualemicillofilho8049 2 месяца назад

    Obrigado irmão um grande abraço aqui do Brasil

  • @joaoqpapelaocoisavelhapidi6175
    @joaoqpapelaocoisavelhapidi6175 2 месяца назад

    Cara você é muito bom parabéns pelo seu vídeo ❤

  • @cabulingue
    @cabulingue 2 месяца назад

    damn Ure jenius Mate

  • @peteoneill5799
    @peteoneill5799 2 месяца назад +1

    This is some proper caveman science.

  • @frantiseklaluch6605
    @frantiseklaluch6605 2 месяца назад

    Good video, I also just take juicy chips and the rest of boards goes into electronic waste container and big guys play with that...

  • @dirceudepin7755
    @dirceudepin7755 2 месяца назад

    Perfeito!

  • @mehdi.p87
    @mehdi.p87 2 месяца назад +1

    بسیار عالی، ابتکار و خلاقیت فوق‌العاده ای داری میتونی جای دیگه استفاده کنی و درامد مناسبی داشته باشی.
    روشی که تو این ویدئو بود (گلد استریپر) بازدهی پایینی داره از این مقدار متریال 2_3 گرم طلا باید دربیاد . درواقع الان فقط طلای آی سی و بی جی ای درومده مابقی تقریبا صفر. ا

    • @PickyPlans
      @PickyPlans  2 месяца назад +1

      مرسی.
      همه روش هارو کار میکنم من با همین متریال قالکاری هم همین نتیجه رو گرفتم اختلاف زیادی نداشت. طلای پین ها خیلی نازک هستش و به دویست سوت نمیرسه .

    • @mehdi.p87
      @mehdi.p87 2 месяца назад +1

      @@PickyPlans البته وزن دقیق متریال ذکر نکردین و مادربرد جز همو چند تا آی سی و بی جی ای آبکاری پین ها خیلی ناچیز هست، و احتمالا محاسبه تون درست هست. بهترین روش برای مادربرد و بردهای لو گرید دقیقا همین گلداستریپر هست.

    • @PickyPlans
      @PickyPlans  2 месяца назад

      8kg (16 PCs) motherboards mix mostly 1 BGA
      9 PCS DDR RAMs mostly 1 sided ICs
      5 PCS CD ram boards
      6 PCS Graphic cards with BGA
      7 PCS voice cards
      1 piece Hard PCB

  • @user-zm7sy8sy3j
    @user-zm7sy8sy3j 2 месяца назад

    بسیار عالی

  • @user-jy1lb9ng5j
    @user-jy1lb9ng5j 2 месяца назад

    خلاقیتی که تو ویدیو میبینم بی نظیره

    • @PickyPlans
      @PickyPlans  2 месяца назад

      به من لطف دارید ❤️🙏

  • @salihakdag6371
    @salihakdag6371 2 месяца назад

  • @user-wx8rw4qe5f
    @user-wx8rw4qe5f 2 месяца назад

    Hello can you give me information the names of materials from the beginning of the video to the end of the video and thank you the work is very wonderful

    • @PickyPlans
      @PickyPlans  2 месяца назад +1

      Thanks my friend...
      The stripper composition is in this video 👇
      ruclips.net/video/8e2o4S4qt4E/видео.htmlsi=uXuhggf9UXUBZYbm
      (Here i used lime instead of sodium hydroxide)
      And the other materials...flux for melting (sodium hydroxide and borax)

  • @ayhamhafez285
    @ayhamhafez285 2 месяца назад

    Another nice video, try to pyrolyze mother boards and smelt for copper yield

    • @PickyPlans
      @PickyPlans  2 месяца назад

      Thank you, my friend. I'm on the same page. However, I believe I'll need a large-scale pyrolysis setup beforehand.

    • @ayhamhafez285
      @ayhamhafez285 2 месяца назад

      @@PickyPlans you can do a test, pyrolizing can be done with your small furnace, just heat the shredded motherboards into crucible, you can add an iron tube above the top hole of the furnace and make some conductions to make smoke cool down, after finish mix your fluxes with the shredded pyrolized motherboards in the crucible and smelt.

    • @jackmclane1826
      @jackmclane1826 2 месяца назад

      @@ayhamhafez285 Do you need to test this. The process is quite straight forward.. just make sure to heat the stuff high enough to ensure a full decomposition, or you'll poison the surrounding.

  • @julianalcorso5703
    @julianalcorso5703 2 месяца назад

    Excellent as usual. It seems the cost and time far exceeds the return for the stripping process! What stripper do you use?

    • @PickyPlans
      @PickyPlans  2 месяца назад +1

      Thanks mate..
      it's composed of an lixiviant for gold like (thiourea, cyanide or thiosulfate) i prefer cyanide
      And oxidizer like metanitrobenzic acid
      Other additives:
      MBT (mercatobanzothiazole) as inhibitor for copper
      Ph adjustors (Sodium hydroxide, lime ) i use lime
      In this video i talked about this composition
      ruclips.net/video/8e2o4S4qt4E/видео.htmlsi=W2G20h33M2O-EKLA
      In part 1 i made m-nitrobenzoic acid
      ruclips.net/video/hyQns1fdUa0/видео.htmlsi=9uVPwP7C24fXLuLI

    • @julianalcorso5703
      @julianalcorso5703 2 месяца назад

      Thanks mate!!!

  • @knowldedge5012
    @knowldedge5012 2 месяца назад

    Would it be a good idea to have a conical scorification dish and let it settle in it rather than pour it into a conical mould?

    • @PickyPlans
      @PickyPlans  2 месяца назад

      It's a good idea... I think you will have less surface area to wash materials in lead.

  • @justinabrahams9432
    @justinabrahams9432 2 месяца назад

    Very good, but I think it's to much energy wasted on to little material. High grade material or larger scale would be good
    But you are really good at what your doing.

    • @PickyPlans
      @PickyPlans  2 месяца назад

      I agree, I needed to know Pd and Au yield of motherboards. Maybe next time...
      Thank you man.

  • @crazyanime348
    @crazyanime348 Месяц назад +1

    Can I use iron pot as Crucible?????

    • @PickyPlans
      @PickyPlans  Месяц назад +1

      It's not a good idea
      Lead would stick to it.
      Use non-magnetic stainless steel.

    • @OwlTech333
      @OwlTech333 Месяц назад +1

      Lead doesn’t “stick” to iron, lead oxide on the other hand “chews” through it, it does the same thing with stainless steel only more slowly. So it really depends on what are you going to use the crucible for. For melting lead iron is perfect, but for oxidising SS will last longer especially in alkaline medium.

    • @PickyPlans
      @PickyPlans  Месяц назад

      Once, I poured 40 kg of molten lead from a cupellation furnace into an iron bowl serving as the mold (Charge temperature was 700° C). However, upon cooling, I found the lead adhered to the mold, akin to soldering. To retrieve it, I had to remelt the lead. Consequently, I began applying graphite powder to "Blacklead" all iron molds thereafter.

  • @crazyanime348
    @crazyanime348 2 месяца назад

    Which crucible you are using
    I mean it is made up with ????

  • @pasqualemicillofilho8049
    @pasqualemicillofilho8049 2 месяца назад

    Muito bom meu amigo, parabéns qual é a sigla do strinping powder ❤

    • @PickyPlans
      @PickyPlans  2 месяца назад +2

      é composição de cianeto ou tioureia com ácido metanitrobenzico e mercatobanzotiazol aqui está o link para o vídeo ruclips.net/video/8e2o4S4qt4E/видео.htmlsi=xGrlQjnj23FKflBd

    • @pasqualemicillofilho8049
      @pasqualemicillofilho8049 2 месяца назад

      Valeu irmão obrigado pela oportunidade de aprender, um grande abraço aqui do Brasil

    • @PickyPlans
      @PickyPlans  2 месяца назад

      🌹🙏

  • @LimbahElektronikIndonesia
    @LimbahElektronikIndonesia 2 месяца назад

    After watching this video,I believe that you still lossing your gold.Total weight of silver when you add at beginning and weight at the end will count the losses of gold.

    • @PickyPlans
      @PickyPlans  2 месяца назад +1

      The yield is fair enough for about 8 kg of motherboards and a few pieces of PCbs. i used 28 grams silver at start. Few mg lost in the process, besides there is no correlation between silver losses and gold losses. Take look at Bugbee's text book.

    • @LimbahElektronikIndonesia
      @LimbahElektronikIndonesia 2 месяца назад +1

      @@PickyPlans I doing precious metals recovery with similar method.I believe that pyrometallurgy route is the best for E-waste materials.Most critical process is when smelting and cupelling.Good luck.
      I read Bugbee cover to cover.

    • @PickyPlans
      @PickyPlans  2 месяца назад +1

      That's really a great book. You as well mate.

    • @OwlTech333
      @OwlTech333 2 месяца назад

      @@LimbahElektronikIndonesiaGREAT BOOK!

    • @davidwong7258
      @davidwong7258 2 месяца назад

      He directly melting AgCl And lost silver.

  • @user-qi2ks9gl3k
    @user-qi2ks9gl3k 2 месяца назад

    سلام بسیار عالی 👏....سیمانی که برای کوپل استفاده کردید چه نوع سیمانی هست؟

    • @PickyPlans
      @PickyPlans  2 месяца назад

      ممنونم.
      سیمان پرتلند( سیاه) .

    • @user-qi2ks9gl3k
      @user-qi2ks9gl3k 2 месяца назад

      @@PickyPlans تشکر .بنده هم این نوع سیمان استفاده کردم بعد از حرارت خوردن ترک بداشت مشکلش چیه؟

    • @PickyPlans
      @PickyPlans  2 месяца назад

      هنگام فرم دهی حداقل میزان اب استفاده بشه یا اصلا استفاده نشه و با فشار فرم گرد ایجاد بشه

  • @user-jy1lb9ng5j
    @user-jy1lb9ng5j 2 месяца назад

    خلاقیتی که تو ویدیو میبینم بی نظیره